POLYATHACRYLATE
Volume Metric Mass : 1,17-1,20 kg/dm3
Inject Temp. 193-254 C
Inject Pressure : 700-1400 bars
Mould Temp. 45-120 C
Shrinkage : 0,2-0,5%
ETHYLCELLULOSA
Valumetric : 1,09-1,17 kg/dm3
Injection Temp. 177-260 C
Injection Pressure 550-2240 bars
Mould Temp. 40-65 C
Shrinkage 0,5-09 %
CELLULOSA ACATATE
Valumetric : 1,24-1,34 kg/dm3
Injection Temp. 168-254 C
Injection Pressure 560-2240 bars
Mould Temp. 45-50 C
Shrinkage 0,5-0,7 %
PROPLONATE
Valumetric : 1,18-1,24 kg/dm3
Injection Temp. 168-249 C
Injection Pressure 560-2240 bars
Mould Temp. -
Shrinkage 0,1-0,5 %
ACATO BUYRATE
Valumetric : 1,15-1,22 kg/dm3
Injection Temp. 168-240 C
Injection Pressure 560-2240 bars
Mould Temp.65-80 C
Shrinkage 0,2-0,5 %
POLYSTHER CLORATS
Valumetric : 1,4 kg/dm3
Injection Temp. 218-240 C
Injection Pressure 700-1400 bars
Mould Temp. -
Shrinkage 0,4-0,6 %
POLYAMIDE 6/6
Valumetric : 1,09-1,15 kg/dm3
Injection Temp. 243-253 C
Injection Pressure 700-1750 bars
Mould Temp. 70-135 C
Shrinkage 1,5 %
POLYAMIDE 11
Valumetric :1,04 kg/dm3
Injection Temp. 200-225 C
Injection Pressure 500-1500 bars
Mould Temp. -
Shrinkage 0,7-2,5 %
POLYETHYLENE HP
Valumetric : 0,91-0,925 kg/dm3
Injection Temp. 149-260 C
Injection Pressure 550-1050 bars
Mould Temp. 40-60 C
Shrinkage 2-5 %
POLYETHYLENE LP
Valumetric : 0,941-0,965 kg/dm3
Injection Temp. 165-310 C
Injection Pressure 700-1400 bars
Shrinkage 2-5 %
POLYPROPELYLINE
Volumetric Mass : 0,9-0,91 kg/dm3
Injection Temp 199-288 C
Inject Pressure 700-1400 bars
Mould Temp. 70-100 C
Shrinkage 1-2 %
POLYSTYRENE ,STANDART
Valumetric : 1,o4-1,0055 kg/dm3
Injection Temp. 160-320 C
Injection Pressure 700-2100 bars
Mould Temp. 50-65 C
Shrinkage 0,1-0,6 %
POLYSTYRENE,HEAT
Valumetric : 1,06-1,11 kg/dm3
Injection Temp. 180-370 C
Injection Pressure 700-2100 bars
Mould Temp. 80-90 C
Shrinkage 0,1-0,8 %
POLYSTERENE, IMPACT RESISTANT
Valumetric : 0,98-1,10 kg/dm3
Injection Temp. 180-920 C
Injection Pressure 700-2100 bars
Mould Temp. 60-70 C
Shrinkage 0,2-0,8 %
POLYSTERENE ACRYLONNITRILE
Valumetric : 1,075-1,10 kg/dm3
Injection Temp. 180-320 C
Injection Pressure 700-2310 bars
Mould Temp. 60-85 C
Shrinkage 0,2-0,5 %
A B S
Volu metric Mass : 1,01-1,10 kg/dm3
Injecion Temp 180-320 C
Injection Preesure 420-1400 bars
Mould Temp 60 C
Shrinkage 0,3-0,6 %
POLYMETHYLSTYRENE
POLYCARBONATES
Valumetric : 1.2 kg/dm3
Injection Temp. 275-300 C
Injection Pressure 700-2310 bars
Mould Temp. 80-90 C
Shrinkage 0,5-0,7 %
POLYURETHANE
Valumetric : 1,20-1,21
PVC & ACETO CHLOR,RIGID
Volumetric Mass : 1,35-1,45 kg/dm3
Injection Temp. 150-205 C
Injection Pressure 1050-2800 bars
Mould Temp. 70 C
Shrinkage 0,1-0,4 %
PVC & ACETO CHLOR,SOFT
Volumetric Mass : 1,18-1,35 kg/dm3
Injection Temp. 180-195 C
Injection Pressure 560-1750 bars
Mould Temp. 60-70 C
Shrinkage 1-5 %
POLYVINYLDENE CHLORIDE
Volumetric Mass : 1,65-1,72 kg/dm3
Injection Temp. 150-205 C
Injection Pressure 700-2100 bars
Mould Temp. - C
Shrinkage 0,5-2,5 %
POLYAMIDES NYLON GLASS FIBRE
Volumetric Mass : -
Injection Temp. 250-290 C
Inject Pressure >500 bars
Mould Temp. 60-150 C
Shrinkage - %
POLYOXYMETHYLENE
Volumetric Mass : -
Injection Temp. 193-225 C
Injection Pressure -
Mould Temp. 120 C
Shrinkage 1-4 %
POLYAMIDES 11 GLASS FIBRE
Volumetric Mass : 1,25 kg/dm3
Injection Temp. 220-250 C
Injection Pressure : > 1000 bars
Mould Temp 60-90 C
Shrinkage : 0,25-0,55 %